High-temperature gas-cooled reactor helium compatibility studies: results of 10,000-hour exposure of selected alloys in simulated reactor helium

1980 
Work on the HTGR Helium Compatibility Task accomplished during the period March 31, 1977 through September 30, 1979, is documented in this report. Emphasis is on the results and analyses of creep data to 10,000 h and the detailed metallurgical evaluations performed on candidate alloy specimens tested for up to 10,000 h. Long-term creep and unstressed aging data in controlled-impurity helium and in air at 800, 900, and 1000/sup 0/C are reported for alloys included in the program in FY-76, including the wrought solid-solution-strengthened alloys, Hastelloy X, Hastelloy S, RA 333, and HD 556, and the centrifugally cast austenitic alloys, HK 40, Supertherm, Manaurite 36X, Manaurite 36XS, and Manaurite 900.