The influences of Mn and heat-treatment technology on microstructure and mechanical properties of medium-carbon-low-alloy wear-resistant cast steel were investigated. The results show that the hardness first increases and then drops down with the increase of Mn content, and the best hardness is 54HRC with Mn content 1.5%. The impact toughness first increases and then drops down with the increase of Mn content. The hardness and impact toughness first increase and then drop down with the increases of quenching temperature. The optimal impact toughness can be obtaind by quenching at 920°C and tempering at 200°C. Part of lower bainite and residual austenite and mass of tempered martensite are obtaind after tempering.