Abstract The capacity of Acidithiobacillus thiooxidans DMS 11478 to recover the heavy metals contained in the residue obtained from the CARON process has been evaluated. Different bioreactor configurations were studied: a two-stage batch system and two semi-continuous systems (stirred-tank reactor leaching and column leaching). In the two-stage system, 46.8% Co, 36.0% Mg, 26.3% Mn and 22.3% Ni were solubilised after 6 h of contact between the residue and the bacteria-free bioacid. The results obtained with the stirred-tank reactor and the column were similar: 50% of the Mg and Co and 40% of the Mn and Ni were solubilised after thirty one days. The operation in the column reactor allowed the solid–liquid ratio to be increased and the pH to be kept at low values (